鋁卷在出貨前的質量檢驗有什么方法?

來源:http://m.yelang007.com/ 發布時間:2022-04-07

  
  鋁卷廠家生產鋁卷之后,要對成品進行檢驗,這是板材生產出貨前的一道工序。那么鋁卷在出貨前的質量檢驗有什么方法?這個問題值得大家來了解了解。
  Aluminum coil manufacturers after the production of aluminum coil, to test the finished product, this is a process before the production and shipment of plate. So what is the method of quality inspection of aluminum coil before shipment? This is a question worth exploring.
  在經過大量的加工過程后,不可避免地會產生各種缺陷和廢品。因此,按照相關標準來檢測板材的尺寸精度和表面質量。超出標準規定的尺寸偏差對成品板材表面應進行光潔處理,邊緣不得有毛刺、裂紋、折角、磕碰等現象。表面缺陷須符合標準規定,須符合相關標準或技術條件的規定,并且光潔、無擦傷、劃傷等。
  After a large number of processing process, it will inevitably produce various defects and waste products. Therefore, in accordance with the relevant standards to detect the size of the sheet and surface quality. Beyond the standard size deviation of the finished plate surface should be smooth processing, the edge shall not have burr, crack, fold Angle, knock against and other phenomena. The surface defects shall meet the standards, the relevant standards or technical conditions, and be smooth, free from scratches, scratches, etc.
  平直度檢驗鋼板表面質量的方法是將受檢鋼板放置在檢驗平臺上,用肉眼檢查鋼板表面是否有超出標準規定的缺陷,再檢查板材與平臺之間的間隙,不超過標準規定范圍的,即為合格成品。將合格的板材一端頭打上合號、狀態代號、厚度、批號、順序號和合格檢印等。
  The method of flatness inspection of surface quality of steel plate is to place the inspected steel plate on the inspection platform, check whether the surface of the steel plate has defects beyond the standard with the naked eye, and then check the gap between the plate and the platform. If it does not exceed the standard, it is qualified finished product. Alloy number, status code, thickness, batch number, serial number and qualified check mark shall be marked on one end of the qualified plate.


  鋁卷生產廠家認為為檢驗成品板的機械性能、內部組織、工藝性能等,須按照標準和工藝規定的項目,對每一批次的產品進行切割試驗,以保證板材的質量符合產品標準,滿足用戶的使用要求。
  Aluminum coil manufacturers think that in order to test the mechanical properties, internal organization, process performance of the finished plate, it is necessary to carry out cutting test on each batch of products in accordance with the standards and process requirements, so as to ensure that the quality of the plate meets the product standards and meet the requirements of users.
  對重要產品的機械性能進行測試。如果在機械性能測試中發現一種樣品不合格,則對該不合格樣品的板材進行二次重復試驗。若再試樣中仍有一件不合格,則報廢。供方可逐張復驗不合格樣品所代表的一段板材。交貨合格,不合格者視為無效。
  Test mechanical properties of important products. If a sample is found to be unqualified during the mechanical property test, a second repeat test is carried out on the plate of the unqualified sample. If there is still one unqualified sample, it will be scrapped. The supplier may retest one sheet at a time the section represented by the nonconforming sample. Unqualified delivery shall be deemed invalid.
  按照國家標準、行業標準、企業標準、技術條件、技術規程等規定,對產品的表面、機械性能等進行全面檢查驗收,確保向用戶提供優質鋁卷產品。更多內容就來網站m.yelang007.com咨詢吧!
  In accordance with national standards, industrial standards, enterprise standards, technical conditions, technical regulations and other provisions, we carry out a comprehensive inspection and acceptance of the surface and mechanical properties of the products to ensure that we provide users with high-quality aluminum coil products. More content to the website m.yelang007.com consultation!

主站蜘蛛池模板: 国产av一区二区三区传媒| 精品伊人久久大线蕉色首页| 午夜精品久久久久久久无码| 国产裸体xxxx视频在线播放| 亚洲 中文字幕 日韩 无码| 四虎成人精品永久在线视频| 精品亚洲一区二区三区在线观看| 级毛片内射视频| 亚洲成a人v欧美综合天堂下载| 免费av在线| 男人国产av天堂www麻豆| 69国产成人精品午夜福中文| 樱桃视频影视在线观看免费| 国产内射老熟女aaaa| av一区二区三区人妻少妇| 亚洲av无码专区在线播放中文 | 久久综合伊人| 日韩在线永久免费播放| 亚洲精品美女久久777777| 亚洲精品无码专区| 自愉自愉产区二十四区| 亚洲精品成人无码中文毛片不卡 | 97人洗澡人人澡人人爽人人模| 成人激情五月天| 久久综合久久鬼色| 人妻丰满熟妇aⅴ无码| 色屁屁www影院免费观看| 97久久精品人人做人人爽| 办公室撕开奶罩揉吮奶头h文视频| 国产精品久久国产精麻豆99网站| 亚洲色18禁成人网站www| 朋友新婚人妻无套| 性欧美xxxx| 少妇放荡的呻吟干柴烈火动漫| 日韩精品无码一本二本三本色 | 国产精品区免费视频| 精品无人区无码乱码毛片国产| 看av免费毛片手机播放| 少妇无码一区二区三区免费| 国产+高潮+白浆+无码| 在线看片免费人成视频久网下载|